Nippon Yakin Kogyo Co., Ltd
Nippon Yakin Kogyo NAS625 Corrosion Resistant Alloys
Manufacturer: Nippon Yakin Kogyo Co., Ltd
Model : NAS625
NAS625 (UNS N06625)
Corrosion-Resistant and Heat-Resistant Nickel Alloy
NAS625 (NCF625, UNS N06625) is a nickel-chromium-molybdenum alloy with an addition of niobium. Matrix stiffening provided by molybdenum and niobium results in high strength. The alloy resists a wide range of severe corrosion environments. It also offers resistance to high temperatures. Uses include parts in chemical and garbage incinerator plants. Nippon Yakin supplies this product in plate, sheet, and strip forms.
Chemical Composition | 62Ni 22Cr 9Mo 3.7Nb 0.71Ti 0.24Al | ||
Product shape | Coil | Sheet | Plate |
Workability | High-temperature strength is much higher than Type 304. Care needed when hot working. Cold workability is similar to standard austenitic stainless steels like Type 304, 316, 316, etc. The high strength needs to be considered in cold working. | ||
Weldability | Shielded metal arc welding, TIG welding, plasma welding are possible. Susceptibility to solidification cracking is higher than Type 304. | ||
Heat Treatment | Solution annealing at 871°C, followed by quenching in water or rapid cooling. For higher temperature annealing, 1030°C followed by rapid quenching. | ||
Pickling | Nitric acid and hydrofluoric acid used in pickling. Descaling more difficult than Type 304, requires alkaline immersion before pickling, blasting also effective. | ||
Applications | Chemical plants, Environment-related equipment, Oil and gas extraction. | ||
Chemical Composition | 62Ni 22Cr 9Mo 3.7Nb 0.71Ti 0.24Al |
Grade/Standard
Nippon Yakin Grade | JIS G 4902 | ASTM B443 | EN |
---|---|---|---|
NAS625 | NCF625 | UNS N06625 | — |
Chemical Composition
C | Si | Mn | P | S | Ni | Cr | Mo | Al | Ti | Fe | Co | Nb+Ta | |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Specification (NCF625) | ≤0.10 | ≤0.50 | ≤0.50 | ≤0.015 | ≤0.015 | ≥58.00 | 20.00-23.00 | 8.00-10.00 | ≤0.40 | ≤0.40 | ≤5.00 | — | 3.15-4.15 |
Specification (UNS N06625) | ≤0.10 | ≤0.50 | ≤0.50 | ≤0.015 | ≤0.015 | ≥58.00 | 20.00-23.00 | 8.00-10.00 | ≤0.40 | ≤0.40 | ≤5.00 | ≤1.0 | 3.15-4.15 |
Physical Properties
Density [g/cm³] | 8.44 |
---|---|
Specific heat [J/kg•K] | 407 |
Electrical resistivity [μΩ•cm] | 124 |
Thermal conductivity [W/m•K] | 9.8 |
Average coefficient of thermal expansion [10⁻⁶/°C] | 30–200°C 13.2 |
30–300°C 13.5 | |
30–400°C 13.9 | |
Young’s modulus [MPa] | 19.7 × 10⁴ |
Magnetism | None |
Melting range [°C] | 1290–1350 |
Mechanical Properties
Mechanical Properties at Room Temperature
Grade 1 (annealed)
Specification | 0.2% proof stress [MPa] | Tensile strength [MPa] | Elongation [%] |
---|---|---|---|
NCF625 (annealing) >0.5mm, ≤3.0mm |
≥415 | ≥830 | ≥30 |
NCF625 (annealing) >3.0mm, ≤57.0mm |
≥380 | ≥784 | ≥30 |
Specification UNS N06625 Grade 1 (annealed) Cold-rolled sheet, strip |
≥414 | ≥827 | ≥30 |
Hot-rolled plate (≤57.0mm) | ≥379 | ≥758 | ≥30 |
Cold-rolled sheet (0.95mm) | ≥276 | ≥759 | ≥30 |
Example Hot-rolled plate 10mm |
399 | 819 | 43 |
Example Cold-rolled sheet 3.0mm |
450 | 859 | 49 |
Grade 2 (solution annealed)
Specification | 0.2% proof stress [MPa] | Tensile strength [MPa] | Elongation [%] |
---|---|---|---|
NCF625 (solution treatment) >0.5mm, ≤70mm |
≥275 | ≥690 | ≥30 |
Specification UNS N06625 Grade 2 (solution annealed) | ≥276 | ≥690 | ≥30 |
Example Hot-rolled plate 10mm |
323 | 738 | 71 |
Example Cold-rolled sheet 3.2mm |
378 | 777 | 59 |
High Temperature Strength
Corrosion Resistance
Pitting Corrosion Resistance
Alloy | ASTM G48 Method A | ASTM G48 Method C Critical pitting corrosion temperature CPT (°C) |
---|---|---|
NAS185N | ○ | 70 |
NAS825 | ○ | 30 |
NAS625* | ○ | 103 |
Test conditions: ASTM G48 Method A (○: No pitting corrosion, X: Pitting corrosion)
– Test solution: 6% FeCl₃
– Test temperature: 22°C, 50°C (Recommended temperature in this test)
– Test time: 72h
*Grade 1
Crevice Corrosion Resistance
Alloy | ASTM G48 Method D Critical crevice corrosion temperature CCT (°C) |
---|---|
NAS185N | 40 |
NAS825 | 45 |
NAS625* | 45 |
Test conditions: ASTM G48 Method D
– Test solution: 6% FeCl₃ + 1% HCl
– Test time: 72h
*Grade 1
Acid Resistance
Alloy | 5% | 10% | 20% | 40% | 60% | 80% |
---|---|---|---|---|---|---|
NAS185N | 0.02 | 0.04 | 1.32 | 2.89 | 3.02 | 4.78 |
NAS825 | 0.01 | 0.03 | 0.32 | 2.21 | 2.24 | 3.73 |
NAS625* | <0.01 | 0.01 | 0.03 | 0.74 | 0.81 | 1.73 |
Test time: 24h
Reference
Alloy | JIS | UNS No. | Chemical composition |
---|---|---|---|
NAS185N | SUS312L | S31254 | 20Cr-18Ni-6Mo-0.8Cu-0.2N |
NAS825 | NCF825 | N08825 | 40Ni-23Cr-3Mo-2Cu-0.7Ti |
NAS625* | NCF625 | N06625 | 62Ni-22Cr-9Mo-3.7Nb-0.2Ti-0.2Al |
Workability
Because the high-temperature strength of NAS625 is extremely higher than that of Type 304, care is required when hot working. The cold workability of NAS625 is basically the same as that of standard austenitic stainless steels such as Type 304, Type 316, etc. However, the fact that this is a high-strength material must be considered in cold working.
Weldability
Various welding methods are applicable in the same manner as with the standard austenitic stainless steels, including shielded metal arc welding, TIG welding, and plasma welding. Susceptibility of NAS625 to solidification cracking is higher than that of Type 304.
Heat Treatment
Annealing of NAS625 is normally performed at 871°C and higher, followed by being quenched in water or rapidly cooled by other means.
Solution annealing of NAS625 is normally performed at 1093°C and higher, followed by being quenched in water or rapidly cooled by other means.
Pickling
A mixture of nitric acid and fluoric acid is used in pickling. However, because descaling is somewhat difficult in comparison with Type 304, alkali immersion before acid pickling, and if possible, shot blasting are extremely effective.
Applications
Chemical plants, Environment-related equipment, Oil and gas extraction.
Related Products
-
Nippon Yakin Kogyo NASHX Heat Resistant Alloys
-
Nippon Yakin Kogyo NASNM15M Non-Magnetic Alloys
-
Nippon Yakin Kogyo NASXM-19 High Strength Stainless Steels
-
Nippon Yakin Kogyo NAS22-3 Controlled Expansion Alloys
-
Nippon Yakin Kogyo NAS21-6 Controlled Expansion Alloys
-
Nippon Yakin Kogyo NASPC Soft Magnetic Alloys